Material Selection and Pre-treatment
Material Specifications: The semi-trailer chassis mainly uses high-strength low-alloy steel (such as Q345B), with a thickness range of 6-12mm (refer to GB/T 1591-2018), and a yield strength of ≥345MPa, ensuring a balance between load-bearing capacity and lightweight design.
Pre-treatment Process: The steel needs to undergo shot blasting (Sa2.5 cleanliness level) and phosphating treatment to enhance the adhesion of subsequent coatings.
Cutting and Forming
Laser/Plasma Cutting: CNC cutting machines (error ±0.5mm) are used for blanking, and a processing allowance of 2-3mm is reserved for key components such as longitudinal beams.
Bending and Punching: Forming is done using a hydraulic bending machine (pressure 800-1200 tons), and the bending radius must be ≥1.5 times the plate thickness (to avoid cracks).
Welding and Assembly
Welding Process: CO₂ gas shielded welding (welding wire ER50-6) is used for longitudinal and transverse beams, and the weld strength must reach more than 90% of the base metal.
Fixtures: Special fixtures are used to ensure that the diagonal deviation of the chassis is ≤3mm (in accordance with QC/T 252-2011 standard).
Heat Treatment and Correction
Stress Relief Annealing: Heated to 600-650℃ and held for 2 hours to eliminate residual welding stress.
Cold Press Correction: Local pressure (≤50 tons) is applied to deformed areas to ensure a flatness error of <2mm/m.
Coating and Corrosion Protection
Primer Spraying: Epoxy zinc-rich primer (dry film thickness ≥60μm), salt spray test ≥500 hours.
Topcoat Process: Polyurethane topcoat (thickness 40-50μm), baking temperature 80-100℃.
Quality Inspection
Non-destructive Testing: Ultrasonic testing is used to randomly inspect welds (proportion ≥10%), and the defect rate must be <0.5%. 2. Load testing: Simulate 1.5 times the rated load (e.g., testing a 40-ton frame with 60 tons) for 24 hours without deformation.